CW602N a dezincification-resistant machining brass, is particularly suitable for use in warm, acidic waters. This material passes the dezincification test according to ISO 6509. For the manufacture of hot-stamped parts C35330 with better hot-working properties is recommended. To achieve dezincification resistance a heat treatment may be necessary after hot working.
CHEMICAL COMPOSITION
Elements | Min Value | Max Value |
Cu | 61.00 | 63.00 |
Pb | 1.70 | 2.80 |
Sn | – | 0.10 |
Fe | – | 0.10 |
As | 0.02 | 0.15 |
Al | – | 0.05 |
Mn | – | 0.10 |
Ni | – | 0.30 |
Total Others | – | 0.20 |
Zn | Remainder |
MECHANICAL PROPERTIES ACCORDING TO EN12164 (AS PER TEMPER R320)
Range (mm) | From | To | UTS Min (N/mm²) | PS Min (N/mm²) | Elongation Min (%) | Hardness Min | Hardness Max |
Round (Dia) | 6 | 40 | 350 | 150 | 25 | 90 | – |
Hex (A/F) | 5 | 35 | 350 | 150 | 25 | 90 | – |
Square (A/F) | 5 | 35 | 350 | 150 | 25 | 90 | – |
PHYSICAL PROPERTIES |
Melting Point | 910°C |
Density | 8.43 g/cm³ |
Specific Heat | 377 |
Thermal conductivity (20°C) | 117 W/m°K |
Thermal expansion coefficient (20-200°C) | 20.7 x 10-6 per °C |
Electrical conductivity | 26 % IACS |
Electrical Resistivity | 0.066 ohm mm²/m |
Modulus of Elasticity | 106 KN/mm² |
FABRICATION PROPERTIES |
Technique | Suitability |
Hot Working Temperature Range | 800-850°C |
Hot Formability | Very good |
Cold Formability | Good |
Machinability rating (free cutting brass = 100) | 75 % |
Annealing Temp. Range | 450-650°C |
Stress Relieving Temp. Range | 250-350°C |
Soldering | Excellent |
Brazing | Good |
Oxy-acetylene welding | Not recommended |
Gas-shielded arc welding | Not recommended |
Resistance welding | Not recommended |
TYPICAL USES